How to Tumble Agates in a Rock Tumbler
Researched guide: written from manufacturer documentation and the sources listed at the end, not from hands-on testing of every product. Some links are affiliate links; see the disclosure.
Agates are the classic tumbling stone. They are hard, they take a high polish, and the banding and translucency that hide under a chalky rind show up once the surface is smooth. They are also forgiving, which makes them a good first batch.
This recipe follows the instructions published by Rocktumbler.com for agate, jasper and petrified wood in a rotary tumbler. If your tumbler’s manual gives different amounts, follow the manual. New to tumbling? Start with rock tumbling for beginners.
Why agates tumble well
- Hardness. Agate sits around 7 on the Mohs scale, the range most tumbling grit schedules are written for.
- Good company. Jasper and other quartz-family stones are similar in hardness, so they can tumble in the same barrel.
- Big payoff. A rough agate often looks like a dull pebble. Polishing reveals the bands, colors and translucency.
The catch is that agates often have pits, cracks and odd shapes. That is why the first stage usually takes longer than the others.
What you need
- A rotary tumbler. Any of the hobby-grade machines in our rock tumbler guide will work, such as the Lortone 3A.
- Rough agate or agates you have collected, about 1/2 inch to 2 1/2 inches across, with a mix of sizes
- A four-step grit kit: 60/90 coarse, 150/220 medium, 500 or finer pre-polish, and an aluminum oxide polish
- Ceramic media to top up the barrel when the rocks shrink
- A plastic colander and bucket for rinsing, and safety glasses for opening the barrel
Before you start: sort the rough
Look over every stone. Set aside pieces that are badly fractured or crumbly, since they break apart and can scratch the rest of the load. Keep a mix of sizes: small pieces fill the gaps between larger ones and help the batch tumble evenly.
The agate recipe
| Stage | Grit | Amount | Time |
|---|---|---|---|
| 1. Coarse | 60/90 silicon carbide | 2 level tbsp per lb of rock | 1 week, usually repeated for a second week |
| 2. Medium | 150/220 silicon carbide | 2 tbsp per lb of rock and media | 1 week |
| 3. Fine | 500 or finer | 2 tbsp per lb | 1 week |
| 4. Polish | Aluminum oxide (TXP or similar) | 2 tbsp per lb | 1 week |
| 5. Burnish (optional) | Water and a little soap | Short run |
Loading the barrel
Fill the barrel about two-thirds full with loose rock. Do not pack it and do not go over two-thirds. Add the grit, then water until it almost reaches the tops of the rocks.
Stage 1: coarse grit
Run the tumbler continuously for a week, then check. Most agate batches get a second week of coarse grit, and two weeks is usually enough for stones up to about 1 1/2 inches. Bigger, harder or misshapen stones can need three weeks or more.
Do not rush this stage. When the stones come out, they should already have the shape you want and no pits or rough patches, just without the shine. Anything left now will still be there at the end.
Stage 2: medium grit
Clean the rocks, barrel and lid completely. The stones will have lost some volume, so add ceramic media if the load has dropped below two-thirds full. Add medium grit and run for a week.
Stage 3: fine grit
Clean everything again. Add fine grit and run for a week. Do not add extra rock or media at this stage. The stones should come out smooth with a satin finish.
Stage 4: polish
Clean very thoroughly. A single grain of coarse grit can scratch the whole batch. Add polish and enough water to almost cover the stones, then run for a week. Nothing else goes in the barrel.
Stage 5: burnish (optional)
If the agates are smooth but not quite glossy, a short run in water with a little grated soap can brighten them. Our grit schedule has the amounts.
Cleaning between stages
Wear safety glasses when you open the barrel; the water is muddy and splashes. Rinse the stones in a plastic colander over a bucket, never in a sink. Used grit and rock mud can clog plumbing. Wash the barrel and lid before the mud dries, because it hardens.
Check each stone between stages. Pull out any that broke or have opened up a cavity, since they can trap grit and carry it into the next stage.
Common agate problems
| Problem | Likely cause | Fix |
|---|---|---|
| Pits or rough spots after polish | Coarse stage too short | Back to stage 1 for another week |
| Fine scratches | Grit carried over | Clean thoroughly, redo stages 3 and 4 |
| Chipped edges | Barrel too empty | Top up with ceramic media to two-thirds |
| Hazy finish | Polish stage contaminated or too short | Clean, rerun polish, then burnish |
Keep a log
Agate batches run for about five weeks, and it is easy to lose track of what went in when. Our free rock tumbling grit schedule has a printable log for dates, grit and notes.
Free printable grit schedule
Grit sizes, times and a tumbling log you can print, plus one short email a week with new guides.
No spam. Unsubscribe anytime. Privacy
Frequently asked questions
How long does it take to tumble agates?
Plan on about five weeks in a rotary tumbler: usually two weeks of coarse grit, then about a week each of medium grit, fine grit and polish. Large, very irregular agates can need three or more weeks in the coarse stage.
How much grit do I use for agates?
The common rule is two level tablespoons of grit per pound of rock for every stage, with water added until it almost reaches the top of the rocks.
Can I tumble agates with jasper?
Yes. Agate and jasper are both quartz-family stones of about the same hardness, around 7 on the Mohs scale, so they wear at a similar rate and can share a barrel.
Why do my agates look dull after polishing?
Usually the coarse stage ended too early, so pits and scratches carried through, or coarse grit contaminated a later stage. Go back to stage 1 or 2, clean everything thoroughly, and work forward again.